Page 1: Differential Scanning Calorimetry (DSC) for polymers/PCR … · 2019. 6. 4. · •Method involves heating a thin film of sample in DSC to 200 oC in nitrogen purge environment (50

1

1 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

Differential Scanning Calorimetry (DSC) for polymers/PCR characterization and applications development

Presented by:

Dr. Rajen PatelDow Packaging and Specialty Plastics

Freeport, Texas

16TH TAPPI EUROPEAN PLACE CONFERENCE

2 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

Homogeneous Polyethylene @  0.920 g/cc.

TEM Micrograph

DSC 

• Peak melting temperature

• Melting distribution

• Weight‐% crystallinity

• Glass transition temperature                    (of amorphous phase)

Page 2: Differential Scanning Calorimetry (DSC) for polymers/PCR … · 2019. 6. 4. · •Method involves heating a thin film of sample in DSC to 200 oC in nitrogen purge environment (50

2

3 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

Polyolefin Characterization Using DSC

• DSC Calibration ‐‐‐ Instrument Baseline & Indium

• DSC cooling and heating rate ‐‐‐ 10 oC/min.

• DSC cooling curve ‐‐‐ Crystallization Onset temperature

Crystallization Peak temperature. 

• DSC melting curve ‐‐‐ Glass transition temperature

Melting Peak temperature

Total heat of Fusion (e.g. ‐20 oC to melting)

Heat of Fusion from 23 oC to melting

Shape of Melting curve (composition distribution)

• ISO 11357‐3 or ASTM D3417‐97 and D3418‐97

4 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

• Temperature Calibration standard

‐ Indium (Onset of melting = 156.6 oC)

• Heat of Fusion Calibration standard

‐ Indium (Heat of Fusion = 28.57 +/‐ 0.17 J/gm)

• Instrument baseline

Calibration of DSC

Page 3: Differential Scanning Calorimetry (DSC) for polymers/PCR … · 2019. 6. 4. · •Method involves heating a thin film of sample in DSC to 200 oC in nitrogen purge environment (50

3

5 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

Indium Calibration – Temperature and Heat of Fusion

IndiumTm = 156.6oCHf = 28.57 +/‐ 0.17 J/gm

156.53 oC28.84 J/g

6 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

Applications of DSC

• Melting and crystallization peak temperatures

• Resin or film crystallinity

• Glass transition temperature (Tg)

• Crystallinity at high temperatures (residual crystallinity)

• Characterization of oxidation induction time (OIT)

• Semi‐quantification of LDPE/LLDPE blends 

• PCR Characterization

Page 4: Differential Scanning Calorimetry (DSC) for polymers/PCR … · 2019. 6. 4. · •Method involves heating a thin film of sample in DSC to 200 oC in nitrogen purge environment (50

4

7 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

Cooled and Heated at 10 oC/min

LLDPE and LDPE resins

0 20 40 60 80 100 120 1400

0.4

0.8

1.2

1.6

2

Temperature (oC)

Heat Flow (Watts/gm)

DOWLEX* 2045

0.920 g/cc

LDPE

0.923 g/cc

109.9 oC

122.4 oC

Could be used in Dish washer

Z-N Octene LLDPE

DSC Comparison of ~0.920 g/cc Polyethylene Resins

8 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

• Lamella thickness determines its melting temperature.

• Gibbs‐Thompson equation

T = TLm m

o e

c f

12

Tm = Observed Melting Temperature in oKTm

o = Equilibrium Melting Temperature = 414.5 K (141.5 oC) for PE

e = Surface Free Energy = 93 ergs/cm2

Lc = Lamella thickness = typically 30 to 300 ÅHf = Heat of Fusion per unit volume 

= 292 x 107 ergs/cc = 292 Joules/cc = 292 Joules/gm

Melting Temperature of Lamella

Page 5: Differential Scanning Calorimetry (DSC) for polymers/PCR … · 2019. 6. 4. · •Method involves heating a thin film of sample in DSC to 200 oC in nitrogen purge environment (50

5

9 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

Melting Temperature vs. Lamella ThicknessPolyethylene Lamellae

0 100 200 300 400 500 60040

60

80

100

120

140

Lamella Thickness (Angstrom)

Melting Temperature (oC)

Melting Temperature vs. Lamella Thickness ( of Polyethylene)

10 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

133.05oC

119.92oC

142.0(146.2)J/g

122.60oC

110.82oC

-20.00oC

23.00oC

4.197J/g

0.0

0.3

0.6

0.9

1.2

1.5

Hea

t Flo

w (

W/g

)

-40 -20 0 20 40 60 80 100 120 140Temperature (oC)Exo Down Universal V2.5H TA Instruments

DSC Second Heat (Z‐N Octene LLDPE)Measured Quick Density @ 23oC  = 0.9207 g/cc

Page 6: Differential Scanning Calorimetry (DSC) for polymers/PCR … · 2019. 6. 4. · •Method involves heating a thin film of sample in DSC to 200 oC in nitrogen purge environment (50

6

11 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

Measurement of Crystallinity

• Density

− Plaque Density (Buoyancy Principle)

− Density Gradient Column 

• Heat of Fusion (DSC)

• X‐ray (WAXD)

These techniques assume a simple two‐phase model for semi‐crystalline polymers 

(amorphous and crystalline phases). 

Since, these techniques measure degree of crystallinity using different principles, 

values measured are usually slightly different for a given polymer.

12 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

Polyethylene Density (Crystallinity)

• Density () = grams/cc @ 23 oC

– Density range ‐ 0.853 g/cc to ~ 0.970 g/cc.

– Density is determined by the percent crystallinity.

» 0.853 g/cc =  0%  Crystallinity

» 0.970 g/cc =  82% Crystallinity

W t% C ry s t . = c a

c a

a=0.853 g/cc

c=1.000 g/cc

Page 7: Differential Scanning Calorimetry (DSC) for polymers/PCR … · 2019. 6. 4. · •Method involves heating a thin film of sample in DSC to 200 oC in nitrogen purge environment (50

7

13 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

133.05oC

119.92oC

142.0(146.2)J/g

122.60oC

112.01oC

-20.00oC

23.00oC

4.197J/g

0.0

0.3

0.6

0.9

1.2

1.5

He

at F

low

(W

/g)

-40 -20 0 20 40 60 80 100 120 140Temperature (oC)Exo Down Universal V2.5H TA Instruments

Heat of Fusion @ 23oC = 142.0 J/gm 

Wt% Crystallinity @ 23oC = 142.0/292*100=  48.6 wt%

DSC Second Heat (Z‐N Octene LLDPE)

Measured Quick Density @ 23oC  = 0.9207 g/cc

Wt% Crystallinity = 50% From Density

14 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

84.75oC

58.41oC

33.20(46.52)J/g

-30.00oC

23.00oC

13.32J/g

0.3

0.4

0.5

0.6

Hea

t Flo

w (

W/g

)

-40 -20 0 20 40 60 80 100 120 140Temperature (oC)Exo Down Universal V2.5H TA Instruments

DSC Second Heat (Polyolefin Elastomer)

Measured Quick Density @ 23oC=0.870 g/cc

Heat of Fusion = 33.2 J/gm @ 23 oC

Wt% Crystallinity = 33.2/2.92@ 23 oC           =  11.4%

Wt% Crystallinity = 13.3% From Density

Page 8: Differential Scanning Calorimetry (DSC) for polymers/PCR … · 2019. 6. 4. · •Method involves heating a thin film of sample in DSC to 200 oC in nitrogen purge environment (50

8

15 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

Wt.% Crystallinity from DSC vs. ASTM Annealed Density

0.84 0.86 0.88 0.9 0.92 0.94 0.96 0.980

10

20

30

40

50

60

70

80

0

20

40

60

80

Annealed Density (g/cc)

Wt.% Crystallinity from DSC

Single Site

PE

Singel Site

PE

LDPE

LLDPE

Wt% Crystallinity

From Density

Wt% Crystallinity from DSC =690.9*den.-589.3

Perkin-Elmer DSC-7

Weight‐% Crystallinity from DSC vs. ASTM Annealed Density

16 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

-90 -70 -50 -30 -10 10 30 50 70 90 110 130

Temperature (oC)

Tg = ‐ 54 oC (Glass Transition Temperature)

-40 oC

87.3 oC

58.7 oC

23 oC

Glass Transition Temperature ‐ DSC Melting Endotherm1 MI, 0.87 g/cc, Octene Polyolefin Elastomer (POE)

Cooled and heated at 10 oC/min

Page 9: Differential Scanning Calorimetry (DSC) for polymers/PCR … · 2019. 6. 4. · •Method involves heating a thin film of sample in DSC to 200 oC in nitrogen purge environment (50

9

17 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

-120 -80 -40 0 40 800

0.1

0.2

0.3

0.4

0.5

0.6

0.7

TEMPERATURE (oC)

TAN(DELTA)

0.859 g/cc

0.8635 g/cc

0.875 g/cc

0.879 g/cc

0.898 g/cc

0.909 g/cc

0.944 g/cc

Gamma Transition

Alpha Transition

Beta (Glass) Transition

Glass Transition Temperature of Ethylene‐Octene Copolymers (DMTA)

18 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

0.86 0.88 0.9 0.92 0.94 0.96-60

-50

-40

-30

-20

-10

0

Annealed Density (g/cc)

Glass Transition Temp. (oC)

DSC (10oC/min)

DMTA Peak tan(delta) (Beta Transition), 10 Rad/s

Glass Transition Temperature of Ethylene‐Octene Copolymers

Page 10: Differential Scanning Calorimetry (DSC) for polymers/PCR … · 2019. 6. 4. · •Method involves heating a thin film of sample in DSC to 200 oC in nitrogen purge environment (50

10

19 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

• Obtained from partial area calculations.

• Useful for characterizing resin melting behavior.

• Useful for understanding various applications such as sealants, shrink film, durable applications requiring high temperature performance, etc.

• Shrinkage ‐‐ inversely related to film residual crystallinity at a given temperature.

Seal initiation temp. ‐‐ temp. at which a critical amount of residual crystallinity is obtained.

High temperature performance  ‐‐ Mechanical properties at a given temperature depend upon residual crystallinity at that temp. 

DSC Residual Crystallinity

20 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

DSC Residual Crystallinity (@ 90oC)

Wt% Crystallinity @ 90oC = 102.8/292*100=  35.2 wt%

Page 11: Differential Scanning Calorimetry (DSC) for polymers/PCR … · 2019. 6. 4. · •Method involves heating a thin film of sample in DSC to 200 oC in nitrogen purge environment (50

11

21 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

Wt% Crystallinity @ 110oC = 58.7/292*100=  20.1 wt%

DSC Residual Crystallinity (@ 110oC)

22 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

• Based on ASTM method D 3895 (ISO 11357‐6:2008).

• OIT is a relative measure of the degree of oxidative stability of the material.

– OIT is primarily determined by amount of primary antioxidants (Phenolic AO)

• Method involves heating a thin film of sample in DSC to 200 oC  in nitrogen purge 

environment (50 cc/min).  Once temperature equilibrium has been established, 

purge gas is changed from nitrogen to oxygen (50 cc/min).  The changeover point 

is considered the zero time of the experiment.  Continue isothermal operation 

until well past the onset of the oxidative exotherm.

• Fast method to quantify oxidative stability of Polyolefin & PCR

DSC – Oxidation Induction Time (OIT)

Page 12: Differential Scanning Calorimetry (DSC) for polymers/PCR … · 2019. 6. 4. · •Method involves heating a thin film of sample in DSC to 200 oC in nitrogen purge environment (50

12

23 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

DSC ‐ Oxygen Induction Time (OIT)

200oC

OIT ~ 11 min.

24 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

• Blend density is given by :‐

• LDPE density (1) can be estimated from the melting point of LDPE fraction.  Z‐N 

LLDPE melting point is almost independent of density.

• Blend density (b) can be estimated from overall heat of fusion. 

• W1 and 2 are unknown and can not be determined.  Need reference DSC curves.

1 11

1

1

2 b

w w

LLDPE‐LDPE Blends Quantification

Page 13: Differential Scanning Calorimetry (DSC) for polymers/PCR … · 2019. 6. 4. · •Method involves heating a thin film of sample in DSC to 200 oC in nitrogen purge environment (50

13

25 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

Tubular LDPE (1.9 MI, 0.921 g/cc)

26 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

Z‐N Butene LLDPE (1 MI, 0.918 g/cc)

Page 14: Differential Scanning Calorimetry (DSC) for polymers/PCR … · 2019. 6. 4. · •Method involves heating a thin film of sample in DSC to 200 oC in nitrogen purge environment (50

14

27 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

80/20 LLDPE/LDPE blend

28 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

60/40 LLDPE/LDPE blend

Page 15: Differential Scanning Calorimetry (DSC) for polymers/PCR … · 2019. 6. 4. · •Method involves heating a thin film of sample in DSC to 200 oC in nitrogen purge environment (50

15

29 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

40/60 LLDPE/LDPE blend

30 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

20/80 LLDPE/LDPE blend

Page 16: Differential Scanning Calorimetry (DSC) for polymers/PCR … · 2019. 6. 4. · •Method involves heating a thin film of sample in DSC to 200 oC in nitrogen purge environment (50

16

31 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

DSC of PE/PP Blend or Co‐ex – How to Calculate PE/PP Ratio ?

• Drop perpendicular at 140oC• Only PP contributes to heat of fusion 

above 140oC• Heat of fusion above 140oC = 56.5 J/g

32 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

DSC of 100% Polypropylene (PP)

178.36°C

162.09°C

93.18(112.6)J/g0.00°C

140.00°C

19.46J/g

0.0

0.4

0.8

1.2

1.6

2.0

Hea

t F

low

(W

/g)

-40 -20 0 20 40 60 80 100 120 140 160 180 200 220

Temperature (°C)Exo Down Universal V4.5A TA Instruments

• DSC of 100% PP reference• Drop perpendicular at 140oC• Heat of fusion above 140oC = 93.2 J/g

Page 17: Differential Scanning Calorimetry (DSC) for polymers/PCR … · 2019. 6. 4. · •Method involves heating a thin film of sample in DSC to 200 oC in nitrogen purge environment (50

17

33 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

DSC of PE/PP Blend or Co‐ex – How to Calculate PE/PP Ratio ?

• Drop perpendicular at 140oC• Only PP contributes to heat of fusion 

above 140oC• Heat of fusion above 140oC = 56.5 J/g• Wt% PP = 56.5/93.2 =  60.6%• Wt% PE = 100 – 60.6 = 39.4%

34 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

DSC Characterization of PCR

Page 18: Differential Scanning Calorimetry (DSC) for polymers/PCR … · 2019. 6. 4. · •Method involves heating a thin film of sample in DSC to 200 oC in nitrogen purge environment (50

18

35 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

DSC of PCR #1 (HDPE)

Wt% Cryst. = 222.4/292*100= 76.2%~ 0.961 g/cc

36 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

DSC of PCR #2 (HDPE)

Wt% Cryst. = 220.6/292*100= 75.5%~ 0.960 g/cc

Page 19: Differential Scanning Calorimetry (DSC) for polymers/PCR … · 2019. 6. 4. · •Method involves heating a thin film of sample in DSC to 200 oC in nitrogen purge environment (50

19

37 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

DSC of PCR #3 (Lot A)

Wt% Cryst. = 151.7/292*100= 52%~ 0.921 g/cc

hPP contamination

38 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

DSC of PCR #3 (Lot B)

Wt% Cryst. = 153.4/292*100= 52.5%~ 0.922 g/cc

hPP contamination

Page 20: Differential Scanning Calorimetry (DSC) for polymers/PCR … · 2019. 6. 4. · •Method involves heating a thin film of sample in DSC to 200 oC in nitrogen purge environment (50

20

39 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

DSC of PCR #4

Wt% Cryst. = 147.9/292*100= 50.6%~ 0.920 g/cc

hPP contamination

40 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

DSC of PCR #5

Wt% Cryst. = 144.5/292*100= 49.5%~ 0.919 g/cc

RCP contamination

Page 21: Differential Scanning Calorimetry (DSC) for polymers/PCR … · 2019. 6. 4. · •Method involves heating a thin film of sample in DSC to 200 oC in nitrogen purge environment (50

21

41 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

DSC of PCR #6

Wt% Cryst. = 145.2/292*100= 49.7%~ 0.920 g/cc

No PP contamination

42 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

Commercial Fabrication Processes Use Fast Cooling RatesBlown film line

Cast film line

Injection molding

1) Fill

2) Cool

3) Open

4) Eject

http://uakron.edu

http://www.eastman.com

http://flexpack.info

102 to 103 oC/s rates are common

additional processing

Chill rolls

Page 22: Differential Scanning Calorimetry (DSC) for polymers/PCR … · 2019. 6. 4. · •Method involves heating a thin film of sample in DSC to 200 oC in nitrogen purge environment (50

22

43 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

Flash DSC (Chip Calorimetry) vs. Conventional DSC

0.5 mm

Parameter DSC Flash DSC

Max Heating Rate (°C/min) 100 3000000

Max Cooling Rate (°C/min) ~60 240000

Typical Sample Size (mg) 2‐10 0.01‐0.2

Flash DSC

Reference

Sample

Entire DSC cell on a chip:

Ability to approach rates comparable to or faster than commercial processing/fabrication conditions to study kinetic processes (e.g. crystallization).

44 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

• Thermal properties are very important in polyolefins/polymer characterization, product research and applications development

• Differential Scanning Calorimetry (DSC) is a  primary tool for characterization of polyolefins, including PCR characterization

• DSC is also an effective tool for characterization and           semi‐quantification of polyolefin blends/PCR

Summary

Page 23: Differential Scanning Calorimetry (DSC) for polymers/PCR … · 2019. 6. 4. · •Method involves heating a thin film of sample in DSC to 200 oC in nitrogen purge environment (50

23

45 Rajen Patel – DSC for polymers/PCR characterization and applications development - 17th TAPPI European PLACE Conference 2019 Porto - Session 14 - Paper 2

Thank YouPresented by:

Dr. Rajen Patel Dow Packaging and Specialty PlasticsFreeport, [email protected]