  • NBSIR 73-103

    Stress Corrosion Behavior of High

    Strength Corrosion Resistant Materials

    E. Escatante and W. F. Gerhold

    Corrosion Section

    National Bureau of Standards

    Washington, D. C. 20234

    February 7, 1973

    Prepared for

    Materials Division

    Naval Air Systems CommandDepartment of the Navy

  • NBSIR 73-103

    STRESS CORROSION BEHAVIOR OF HIGH

    STRENGTH CORROSION RESISTANT MATERIALS

    E. Escalante and W. F. Gerhold

    Corrosion Section

    Metallurgy Division

    February 7, 1973

    Prepared for

    Materials Division

    Naval Air Systems Command

    Department of the Navy

    U. S. DEPARTMENT OF COMMERCE, Frederick B. Dent, Secretary

    NATIONAL BUREAU OF STANDARDS, Richard W. Roberts, Director

  • Progress Report

    on

    Stress Corrosion Behavior of High StrengthCorrosion Resistant Materials

    E. Escalante and W. F. GerholdCorrosion Section

    Metallurgy Division

    Results to date in the investigation of the stress -corrosion behaviorof high strength corrosion resistant materials (authorized under RRMA 2007)are included herein.

    The materials that are being studied in this investigation includethe following:

    Alloy Steels

    PH 14-4 Mo, "C "-ringsPH 14-8 Mo, sheet17-4 PH, sheet17-4 PH, forgingPH 15-7 Mo, sheetAM 350, sheetAM 355, sheetAM 355, wireAM 357, sheet17-7 PH, sheet17-7 PH, wireThermenol , sheetA 286, sheetHNM, sheet17 Cr-5 Ni, foilCustom 450Custom 455

    Titanium Alloys

    6 A1-4VC105 VAA110 ATCI 15 VAB120 VCA

    The tests are being conducted in the marine atmosphere at the SO' and

    800' lots at Kure Beach, North Carolina. Table 1 and Table 2 contain the

    results obtained from tests conducted at the 80' and the 800' lots, respec-

    tively.

    These tests are continuing.

  • '

    a>CC} ?Hf-i cd -H

    2

    r--

    r—2 »

    i—t o>«t LO LOr-^ (Ni

    ct! ^ca, cd

    PC u. tu2 2 Z 2o. f*.

    r-» r---

    /—\ /—\ v£> —

    I

    •-—1 ^—' O tOH

    CN]

    o00

    /—

    \

    00 MDO v—

    '

    r—I •>+J 2 oo 1

    CD r-» m3to tO CN1 tOX 3 PC » p-.ti.y-i U-, P., v

    y -\

    aj rH 2 2 2 2 2 2 2 CNJ LOa -h /— /—> 00 /—-s /—-\ /—

    \

    /—v /—\ r—\ LOcd tO N H M K) to to to sD totu v t v / ^

    [ 1—1 *rj" r-» r-. to Lf) (N N CM CO (M H 00 CNJ (NJN O O)

    ooO MO toto LO

    to 00 tJ-(NJ ttJ- V.O

    r-l r-t 00 I—

    I

    CNJ 00 r—4 tOr-l rH CNJ COE-1 co

    0 >Hfn

    3co OOPho\°XUJ

    LO o oN O) O LO o or-~ o LO o or~-~ ct> o O LO o oCO N CTl O O LO O OLn n oi o

    +->

    CD

    S+->

    ct5

    CD

    fn

    *3

    cc!

    •Hr-t

    CD+->

    CC5

    CO00G•H Ph tufn o cro oo oy a> o

    4->

    I—

    I

    _+-)

    o aj r

    CD T3rH CD

    CD !hCD

    rH ItCD

    X E- CDH

    Ph

    oo

    +->

    ccj :

    3CD

    rHCD

    CD

    H

    o oLO LOo orH Z - - rH

    RH

    CO

  • 3

    > -h< Q CTJ

    XI X) X> XJ X> X) X X X X X X X .£> vO Ci (N

    O ^+->

    i

    CO

    CO

    - \DMD i—

    (

    " /—

    *

    •> LO tOCO i—< v—

    '

    LO - LO"> , ^ i—l

    O M •>(M ^—' tO ^

    *» LO r—( LOCT) « -> v—

    '

    •-h

    tn

    CT>o lo r~- o lo n c oCD >i i—l I—I r-i I—I i-Hu3 4h(/) ooXPJ

  • o oMP d)a uu w 3>,r-H

    > cd -H< a cdPU

    4-1

    o ^MV) Jh

    c3 i—

    i

    a -hctf

    PU

    Xl Tt M Nv >

    i—i -

    rH

    re *3-ai tj-CM •>

    t-l CMi—I «to a>CM i—

    I

    00 00LO CN!

    Ln cm

    CM CM

    CM i-H

    CM \£>CM i-i

    O 00 OXI CM CM 00v_>tO *>r-t»o o

    a» to i-tto •> •>r-H /—\ CT>i—t '—' *O CTl OI—t I—i \01 *y

    00 vOCM r-H CM

    ^ tOX> *tf rQ

    to x—

    '

    CMcr>

    CM

    CTl

    CTl

    CM 00tO 00

    •> i—

    i

    o -LO CM•n- en

    1—1 00CM LO

    /—

  • \£) vO(O H H H rj- CM LO

    CDCO Jh

    ct$ 1-hQ -HPL,

    vD /T-> rHlO CM rt CM

    >—' * tOrs CM fx /—\ /—

    \

    o LOCM CM LO CM CM oo i—

    1

    v ' * •> V J *

    J i—l

    LO O 00 H 00 L/l i—l CMCM CM rH tJ- CM CM o Ol

    o> •» •\ «\ CM rH O00 /"~\ /""N to 00 /—v I—

    V

    r—l

    I—

    1

    vO tO LO \ 1 tO tO CM CM to f—

    \

    I—

    1

    to -> v / v > to to to toto LO vD vO 'it LO 00 00 LO LO v > 1—

    '

    CM tO H H H rH CM i—( i—l r-H i—

    i

    00 1—1 to to to

    +Jcoo

    0rH

    a

    •H -H

    cd tu

    CO T3CD

    O

    o

    oPh> CJ> CM OOr-^ i—i rt- loLO tO 00 r-Hi-i h o torH rH CM CM

    O CM tO toto to to to

    \0 tO CM

    to to to to

    to to to to

    tJ- kO to 00

    CD CD to CT>Is- h i/i CM tO CO T00 CM VD

    to

    to

    a>

    uH->

    coCO

    CD

    rH

    to

    oPL,o\°

    XUJ

    cwo

    O LO o oLO N Ol O O LO o olo cd o oLO LO o oo o O LO o olo r-~ cr> o O

    LO o otO Mj) O

    +->

    c(1)

    £+J

    cd

    fHH

    ct3

    rHCD

    Mcci

    s

    +->

    CDCD

    rCto

    o1—

    I

    rH

    oLOto

  • o +-> cd

    ^ « 3CD X rH> CTJ -H< Q 03

    4hO ^+->

    /»->> r~> '—s /—

    v

    in to lo lov > V I \ I < '

    K) M "t

    CT\ LO to CMCM

    CO

    CM

    toCM LO

    •> i—I /—\ to/—> •> ^J- *>CM /—* *—' /—

    s

    ^ to tovO *—' »> v—

    '

    rH tO CM CM

    CM

    i—\ >—\ r-> loJ3, X) N O

    lo

    toco

    i—I i-HrH

    CM CMOO CMLO i-HCM >« CMO O

    i-H O

    O « vOr- /—% ooCM CM 00

    •» ^— #vvO cn ooo to to00 LO i—

    I

    Xi Xi X)

    to

    cCD

    e+->

    03

    uE-

    o3

    •HrHCD+->

    oj

    2

    CDCD PL, CD

    CD O•H O

    CO O o00 O LO

    l LO oo r z X H - - - O CO z z z rHo CO o OS i-HrH o r-H u i-H XrH i-H 03 oi03 o CT$ o XL0 LO Cl.LO LOto to

    i

    < rH

    LOr--o

    X

  • tpv t

    CO O04 .p CD

    fn (/> 30) X rH> rt -h< Q tj

    Pu

    /—\ cx> ooO O) .-H 00 O 00lo \o voCM

    U-, Ll,

    O". r-H

    NO OtO vO toi-H tO

    oo, to

    r-H "sj* CMO r-H t^-\0 O HtO r-H

    or-H

    CM•> O

    / V cr> oo O CM

  • CD OMP d)^ to 3CD X rH> rt -h< Q cd

    \0 N CiCl M 00

    lo

    LO /—"v CM 00rQ Tf I—

    I

    to r-ito .aLO v—

    '

    X J i

    LO/—

    \

    CTi/—

    V

    rHv—' CM CM r-l

    O v—

    '

    Tf ^^ vD+-» vQ LO to LO

    CD VO 00 tO LO to TfV) ^ tO r-l "tO •> Tf to TfX 3 rH lo CM •> LO \£> i CMCti pH •> i—l c% Tf to r-»Q -H O •> CT> 00 CT>

    c 00 tO r-lrH Tf rH 00 * to to

    •t «fc «k - to •» '—

    '

    CT> o LO Ci^ M Ol LO Tf LO VO vO o> rH TfM vO \£> i—l i—( to Tf to rH tO

    to

    co cd

    to

    o

    T3

    O CtJ

    cdtp toO O

    ft• XO B32

    3

    tO tO CM

    tO tO CM

    LO Tf LO Tf

    LO LO LO LO

    tO rH Tf CM

    Tf Tf Tf Tf

    O O O OLO LO LO LO

    o o o oLO LO LO LO

    o too VI

    v >

    1c

    rH pCO Tf CM Tf 00 Tf vO cr> cn Tf 00 Tf Tf v£> LO CO

    CD •H1—1

    3

    oo3,o\°Xw

    O LO om N O LO o olo r-~ o O LO o o1/1 N CJl O O LO O Olo r*- cn o o LO o oin n o o

    4->

    CD

    6Pce

    CD

    Sh

    H

    C3

    CD

    PaJ

    uI

    Xc_5

    i

    a>

    u

    O -rH PrH CCtS O

    oCu

    i

    oCM

    +-> CD

    CO GOCD CTj

    to1—

    1

    +->

    CD

    CD ai CD -a +j>> C X CD CDo U •H to +-> CDi—

    i

    CD Cfi

    rH 3 = = = totO P ?Hc •H o pH bO 1—1

    o rH C rH c ofi H O a O rHa> rJ •iH i—

    1

    e vO +-> ctSu 00 3o CM i-H

    < So

    oLOto

  • CD o00 +J CD0$ fn?-< co 30) X r-l> rt -h V CD r-l r-l

    •» CN vD >—' » *\0 '—

    '

    CN1 tO CMr-l o /—

    ^

    CM i—l i-H•> r-l

    £!>to « tO CM \0r-l tO to i-H rH 1—1

    t/>

    CD CD

    e•H -Ho rtCD Vu

    CO T3CD

    4-1 CO

    O Ou*

    o tu52

    to to to

    to to to

    to to to

    to to to

    O o oLO ^ LO

    O o oLO ^ LO

    o o o oLO LO LO LO

    o o o oLO LO LO L0

    o coo CO

    N '

    1C

    1—1ol

    CD •Hi—l CD in

    X> U r*cU

    E-

    Expos

    00 o ^ tO LO toi—I O "3- LO Oi"vl" rH LO lo to r-.i—l CM CM i—l CM CM

    O O 00\o cn rf00 CM LO

    Ol Ol 00

    o>O \D CD

    vO tO O (M OO C ^

    00 to LO t**o "5t

    oo to lo r*.

    CO

    CO

    OU ••M COCO • O LO O OLOO OlOO OloO OLOOO O LO o o

    lo n w Lor^cn m n en w n o> lo cn o lo a> oCD >- i—I i-Huco OoOho\=>Xm

    +>

    CD

    ep0

    H

    CcS

    as

    •Hf-i

    CD+->

    2

    o

    O

    LOI

    uu

    13CD

    as :

    U

    oo

    oLO

    eoCO

    u

    ooo

    <co

    >-Sfr

    <

  • 0 O60 P 005 Sh

    f-l (O 30 x ^> CO -H< a R)

    Pc

    ^3 XI 43 X> X) X> X> Xl X)

    tpo wP

    0)

    to Jh

    co i—

    i

    a -hco

    CO

    c *oo 06 «"H•H >HO co0 PCft\CO 13

    0)tpo

    CO

    oft

    pj

    o o o oLO LO LO LO

    o o o oLO LO LO LO

    o o o oLO LO LO LO

    po coo tov—/

    co0 •H1—1 a) to

    X) f-l ^CO 3

    to

    o

    B*PJ

    to

    co

    Vf-i

    4-> COco

    0 >1P3

    vO 00 i—

    I

    CM tOCM

    vO LO CMoo cm i—i r^-

    O0 M Cl N00 to LO c

    O LO o oLO N ffi O O LO o oLf) h- 0~1 O O LO o ol/l N CD O

    P0epco

    0

    E-

    Cco

    co

    •HP. >

    o£ ^ o LO o

    1—

    1

    1—1 CM•H I I—

    1

    1—1 i—l

    CO < 03p•HE-

    oX!co

    to

    cd

    Tj

    tHO

    p0

    pto '7-; CM

    P co

    PLO to

    CM 0t—

    <

    pa> i—i O

    £j I l o

    pp P P

    P p 0

    >c C o•H •H •H £

    0i—l r—

    1

    Pi—l i—

    1

    i

    1 ft•H •H •H •HP P P 0 f-l 010 to to bO cJ5 £

    rf •HCO to to O

    13 O 00 0 0 P ft£ s £ CO P coH •H •H oo O O p XI0 0 0 C 0a, ft ft 0 e pco to to £ 3P i—iP. f-l f-l co to HO o o 0 13 co4-1

  • CD O CDW) P 5h03 3

    m hCD X-H> o3 oi< Q B.

    OONI

    oLOtO

    CM 00CM LO o

    O CD to o-.4-> 5h /—

    \

    CMCM I—

    1

    10 i-l > ' CMX'H i—

    1

    LO«j Cj CM to i-H

    O i-HCM to

    v '

    00 or-H CM •3-

    CD

    5h

    3to

    O

    ouCD

    to cQ -H

    o5h

    CD U•l-l

    5h

    o3

    S

    •r-l

    P5h

    O2

    to

    CD H>

    CD PL,

    CO 13CD

    to 5h CD cop 5-1 5-i •Ht-H O CD COa 5h ^410

    CD to co

    0i CO +-) oCD o &5-1 XP 0JCO oo

    COCMp to

    CD o3 to

    rH CDiJD 5h •

    oJ P COH co

    CD >h

    3

  • 0) O 0)

    > aj cti< Q [i

    CMCM

    o in

    aj

    t- )0S

    o to LO Ol vO vO o a--!—

    1

    to CM Or-l to 1—

    1

    O 00 LO CMr-H 1—

    (

    r-l 1—1 r-H i—

    t

    totO

    UPCO

    CO

    >-

    V) OOX

    LO LO LO LO LO LO1^-

    LO LO1^-

    LO

    +-> +->

    c a>o p oe 0)p Q> to PCS

  • a> o ©60 P f-i«J 3f-l W r-l© x-h> rt< u.

    o ©p f-iW rH

    Q b

    13

    •Ho3

    ©ft-CO 13

    0)

    O

    o2

    Oft

    to

    oLf)

    oLO

    oLO

    oLO

    oLO

    po tou to

    COco

    © >-fn

    t/) Oofto\°X111

    pcsca

    H

    C

    •Hf-l

    0)

    P03

    2

    lo1^

    LO LO

    P©(0

    10

    o

    s3•Hc

    P

    <

    >i

    i—

    i

    <

    <CO

    LOo

    CM LOto to CM to CMi—

    i

    I—

    1

    i—

    1

    T—

    1

    i—i

    i—I C7>

    P P p10 to to

    © © ©p P p

    C c•H •H •H

    i—l i—l T—

    1

    7—1 i—

    (

    1—1

    •H •H •HP P P

    LO LO tO V) in

    tO tO to

    c a© © ©s e sH •H •H -ao O o o© © © 60ft ft ft aj10 10 to ©

    DOfn f-l f-i

    o O o © am ip

    to a) to © P

    o O o 3LO o ft ft ft © r—

    1

    i—l CM X X X •H Oi—l i—( w w 0J Cm COu 03

    oj o ©

  • form NBS-114A H--71)

    U.S. DEPT. OF COMM. I 1. PUBLICATION OR REPORT NO. 2. Gov't AccessionBIBLIOGRAPHIC DATA

    j NBSIR 73-103N°'

    3. Recipient's Accession No.

    4. TITLE AND SUBTITLE

    Progress Report on Stress Corrosion Behavior of HighStrength Corrosion Resistant Materials

    5. Publication Date

    January

    6. Performing Organization Code

    7. AUTHOR(S) _ _ . , „. _ _ i . ,E. Escalante and W. F. Gerhold

    8. Performing Organ i/.mon

    9. PERFORMING ORGANIZATION NAME AND ADDRESS

    NATIONAL BUREAU OF STANDARDSUtrAKlMtlNl Ur LL/MMllK^E.WASHINGTON, D.C. 20234

    10. Hro|cct/T.isk/Work Unit No.

    3120410

    11. Contract/Grant No.

    12. Sponsoring Organization Name and Address

    Materials DivisionNaval Air Systems CommandDepartment of the Navy

    13. Type of Report Si PeriodCovered

    14. Sponsoring Agency Code

    15. SUPPLEMENTARY NOTES

    16. ABSTRACT (A 200-word or less factual summary of most significant information. If document includes a significantbibliography or literature survey, mention it here.)

    This report contains results to date in the investigation of the stress-corrosionbehavior of high strength, corrosion-resistant materials exposed to marineenvironments. These materials are high strength alloy steels and titanium alloysin the form of c-rings, wire, sheet, forgings, and foil. The investigation is stillin progress.

    17. KEY WORDS (Alphabetical order, separated by semicolons) Alloy Steels; high Strength materialsmarine environment; stress .corrosion; titanium alloys.

    18. AVAILABILITY STATEMENT

    UNLIMITED.

    1x1 FOR OFFICIAL DISTRIBUTION. DO NOT RELEASETO NTIS.

    19. SECURITY CLASS(THIS REPORT)

    UNCL ASSIFIED

    20. SECURITY CLASS(THIS PAGE)

    21. NO. OF PAGES

    14

    22. Price

    UNCLASSIFIED

    USCOMM-OC 6