Surface Analysis A.) Introduction:
Solid Surface: the boundary layer between a solid and either a vacuum, a gas or a liquid- differs substantially in its physical properties and chemical
composition relative to the interior of the solid and average composition of the
bulk sample.- not just the top layer of atoms, but a transition layer with non-uniform composition that varies from the outer layer to the bulk.- generally a very tiny fraction of the total solid
Operational Definition: volume of a solid that a particular measurement techniques samples- several surface techniques may sample
different surface
Increasing magnification of the surface of a pin with the presence of bacteria
B.) Spectroscopic Surface Methods: 1. Provide chemical information of the composition of a surface (few to ~ 10s thick)
From source(primary beam)
To Spectrometer(secondary beam)
Sample
- Results from scattering, sputtering or emission.
- Further studied by other spectroscopic techniques
- Photons, electrons, ions or neutral molecules.
- Need to limit to surface analysis
Penetration depth of 1-keV electrons is ~ 25 , where a photon beam of same energy is ~ 104
Method and Common Acronym Primary Beam Secondary Beam
X-ray Photoelectron Spectroscopy (XPS), or Electron Spectroscopy for Chemical Analysis (ESCA)
X-ray photons Electrons
Auger Electron Spectroscopy (AES)Electrons, or X-ray
photonsElectrons
Ultraviolet Photoelectron Spectroscopy (UPS) UV photons Electrons
Secondary Ion Mass Spectrometry (SIMS) Ions Ions
Laser Microbe Mass Spectrometry (LMMS) Photons Ions
Electron Microbe (EM) Electrons X-ray photons
Some Common Types of Spectroscopic Methods for Analysis of Surfaces
Methods are differentiated by the nature of the primary and secondary beams
2. Sampling Surfaces and Contamination- focus beam on a single surface- mapping the surface by scanning the beam across the surface in a raster pattern
‚ can be linear or two-dimensional‚ observe changes in secondary beam as a function of position
- depth profiling etch a hole in the surface by sputtering‚ a finer primary beam is used to generate a secondary beam from the
hole‚ observe changes in secondary beam as a function of depth
Depth Profiling
Raster Pattern(data is obtained from primary
beam centered in each grid)
- contamination of the surface from the atmosphere or the primary beam- need to clean surface in vacuum chamber
‚ bake sample at high temperatures ‚ sputtering the sample with a beam of inert gas ions from electron gun ‚ mechanical scraping or polishing the surface with an abrasive ‚ ultrasonic washing in various solvents ‚ bathing the sample in a reducing atmosphere to remove oxides
Surface contamination
3. Electron Spectroscopy- signal from sample is a beam of electrons (secondary beam)- determine the power of the beam as a function of the energy of the electrons (h)- determine
‚ identification of all elements (except H and He)‚ oxidation state of element‚ type of species element is bonded to‚ electronic structure of molecules
- poor penetration power of electrons‚ restricted to surface layers of 20 – 50
-qualitative analysis of the surfaces of metals, alloys, semiconductors and heterogeneous catalysts
Different element abundance in different regions of the surface
A). Electron Photoelectron Spectroscopy (XPS)i. Theory
- record kinetic energy of emitted electron‚ plot of number of emitted electrons as a function of the energy of the emitted electron
- X-ray beam of known energy (h) displaces an electronA + h A+* + e-
-Kinetic energy of emitted electron (Ek) is measured in an electron spectrometer
‚ Binding energy (Eb) of the electron is:Eb = h - Ek - w
where:h – energy of electron beamEk – measured kinetic energy of emitted electron w – work function of spectrometer (determined
experimentally)
Photoelectric Process
Binding Energy (eV)
Binding Energy of an electron is characteristic of the atom and the orbital from which the electron was emitted
- well separated peaks for each element on the surface can be observed‚ except hydrogen
- observe multiple peaks for each element‚ S, P and D orbital‚ energy decreases as a function of orbital
S > P > D‚ energy increases as a function of atomic number
N1s > C1S
ii. Instrumentation- Expensive ($300,000 - $900,000)- Requires extensive vacuum systems (10-5 to 10-10 torr)- Similar to optical spectrometers
5 4 . 7
X-rayX-raySourceSource
Hemispherical Energy AnalyzerHemispherical Energy Analyzer
Position Sensitive Position Sensitive Detector (PSD)Detector (PSD)
Magnetic ShieldShieldOuter SphereOuter Sphere
Inner SphereInner Sphere
SampleSample
Computer Computer SystemSystem
Analyzer ControlAnalyzer Control
Multi-Channel Multi-Channel Plate Electron Plate Electron MultiplierMultiplierResistive Anode Resistive Anode EncoderEncoder
Lenses for Energy Lenses for Energy Adjustment Adjustment (Retardation)(Retardation)
Lenses for Analysis Lenses for Analysis Area DefinitionArea Definition
Position ComputerPosition Computer
Position Address Position Address ConverterConverter
- X-ray source (X-ray tube)‚ bombardment of a metal target with a beam of high-energy
electrons- electrons produced at heated cathode- accelerated to metal anode, copper block with target
(Mg, Al)- large potential (100 kV)
‚ X-rays produced by decelerated electrons upon collision with target- energy of photon is equal to the difference in kinetic energy
of the electron before and after collision.- deceleration occurs as a series of collisions different kinetic energy losses- X-ray energies vary over a continuum
‚ Very inefficient, less than 1% of electrical power converted to X-rays- remainder dissipated as heat- water cooling is required
- Sample holders‚ samples mounted as close to X-ray source as possible
- avoid attenuation of X-ray‚ sample container under a vacuum (<10-5 torr, typically 10-9 to 10-10
torr)- avoid contamination of sample surface by water or oxygen- avoid attenuation of X-ray beam due to inelastic collisions
- Analyzers‚ hemispherical type‚ electron beam deflected by an electrostatic magnet
- electrons travel in a curved path- radius of curvature is dependent on kinetic energy of electron- vary field, direct electrons of different kinetic energy onto detector.
‚under a vacuum (<10-5 torr)
- Transducer (detector)‚ solid-state, channel electron multipliers‚ tubes of glass doped with lead or vanadium
- apply a potential of several kilovolts across these materials- a cascade of electrons (106 -108) for each incident electron- pulses are counted electronically
‚ similar in concept to photomultiplier tubes
iii. Chemical Shifts and Oxidation States- position of a peak is dependent on the chemical environment of the atom- variations in the number of valence electrons and type of bond influence the
binding energy of the core electrons
FunctionalGroup
Binding Energy(eV)
hydrocarbon C-H, C -C 285.0
amine C-N 286.0
alcohol, ether C-O-H, C -O-C 286.5
Cl bound to C C-Cl 286.5
F bound to C C-F 287.8
carbonyl C=O 288.0
Binding energy increases as a function of electronegativitySimilar effects observed for different Oxidation states
Similar effects observed for different Oxidation states
Element Oxidation State
-2 -1 0 +1 +2 +3 +4 +5 +6 +7
Nitrogen (1s) - *0 - +4.5 - +5.1 - +8.0 - -
Sulfur (1s) -2.0 - *0 - - - +4.5 - +5.8 -
Chlorine (2p) - *0 - - - +3.8 - +7.1 - +9.5
Copper (1s) - - *0 +0.7 +4.4 - - - - -
Iodine (4s) - *0 - - - - - +5.3 - +6.5
Europium (3d) - - - - *0 +9.6 - - - -
Electron volts relative to oxidation state marked by *
B). Auger Electron Spectroscopy (AES)i. Theory
- two-step process, generates Auger electron‚ differs from XPS
1) generate excited ion as before:A + h A+* + e-
or using an electron beamA + ei
- A+* + ei’- + eA
-
where: ei
’- is the beam electron after interaction with A and loss
of kinetic energy. eA
- is ejected from A inner orbital2) excited ion may relax by emitting an Auger electron (eA
-) with
kinetic energy (Ek)A+* A++ + eA
-
or by fluorescence (X-ray fluorescence)A+* A+ + hf
-Kinetic energy of emitted electron (Ek) is independent of the energy of photon or electron that ‚ Kinetic energy (EK) of the Auger electron is:
EK = (Eb – Eb’) – E’b = Eb – 2Eb’ where:
(Eb-Eb’) – energy released in relaxation of the excited ion Eb’ – energy required to remove the second electron from
its orbit
- Auger emissions are described in terms of the type of orbital transitions involved in the production of an electron ‚ KLL:
1. removes a K electron2. transition of an L electron to the K orbital 3. ejection of a second L electron
‚ LMM and MNN are also common transition- measurement of the kinetic energies of the emitted electrons
‚ each element in a sample being studied will give rise to a characteristic spectrum of peaks at various kinetic energies.
‚ Spectra typically displayed as a derivative (dN(E)/dE) - enhance small peaks, repress effects of intense peaks
- Auger electron emission and X-ray fluorescence are competitive processes‚ lower atomic number Auger electron emission‚ higher atomic number X-ray fluorescence
AES Sample: Pd Ep = 2.5 Kev
ii. Advantages- sensitivity to atoms of low atomic number
- minimal matrix effects- high spatial resolution‚ detailed examination of solid surfaces
‚ electron beam more tightly focused than X-ray beam
iii. Disadvantages- not used to provide structural and oxidative state information (XPS) - quantitative analysis is difficult
iv. Instrumentation- similar to XPS, most instruments do both XPS and AES
- requires an electron gun
Diagram of Electron Gun
-Heated tungsten filament•0.1 mm diameter•Bent into shape of hairpin with V- shaped tip• maintained at potential of 1 -50 kV
-Wehnelt cylinder• surrounds filament• negative bias to filament (0-3000V)
- electric field of Gun causes electrons to converge at crossover-Produces a beam of electrons of 1 to 10 keV
• can be focused onto the surface with diameters of 500 to 5 m
4. Scanning Electron Microscopy- high resolution images of surfaces
‚ optical microscopy limited by wavelength of light, diffraction
effects- surface is swept in raster pattern with finely focused beam of
electrons‚ swept in straight line in x-direction‚ returned to starting point‚ shifted downward (y direction) by a standard direction
Cecropia Moth Scales (15,000x)Cecropia Moth Scales (350x)
A). Scanning Electron Microscope (SEM)i. Introduction
- surface is scanned with beam of electrons- several types of signals from the surface are created
‚ backscattered or secondary electrons- two most common for SEM ‚ X-ray fluorescence‚ Auger electrons
-Condensing lens and objective lens reduce electron beam to final spot of 5 to 200 nm
-Two magnet coils in objective lens deflect e- beam in x and y direction to scan surface
- intensity of beam created from surface are used to drive the horizontal and vertical scans of a cathode-ray tube (CRT).
-Magnification (M) = W/w where:
W – width of CRTw – width of single line scan across the sample
- increased magnification is achieved by decreasing w‚ narrower the beam of electrons the higher the magnification
‚ magnification range is 10x to 100,000x
Increasing Magnification of Mosquito
- samples changers are designed for rapid changing of samples‚ large-capacity vacuum pumps bring pressure to < 10-4 torr
‚ can hold samples many centimeters in length‚ can be moved in x, y and z directions
- sample considerations‚ samples that can conduct electricity are easiest to study
- flow of electrons to ground minimize artifacts- also typically good conductors of heat- minimize thermal degradation
‚ most biological and mineral samples do not conduct electricity- coat surface with thin metallic film by sputtering or vacuum evaporation
- detectors ‚ scintillation device
- doped glass or plastic emits photons when struck by electrons
- detectors ‚ scintillation device
- doped glass or plastic emits photons when struck by electrons
- photons conducted by light tube to photomultiplier tube (outside
instrument)- gains in signal of 105 to 106ii. Interaction of Electron Beams with Surface
- elastic interactions‚ affect the trajectory of electron not energy‚ deflection of collision is random (0 to 180 deg.)‚ beam penetrates to a depth of 1.5 m or more‚ eventually exit from surface as backscattered electrons- larger diameter limits resolution
- inelastic interactions‚ transfer part or all of energy from electron to solid‚ excited solid emits secondary electrons, Auger electrons, X-rays
Simulation of Electron Trajectories
- Secondary Electron Production‚ electrons having energies of 50 keV or less are emitted from surface
- along with backscattered electrons - ½ to 1/5 number of backscattered electrons
‚ beam ejects conduction band electrons‚ only from depth of 50 to 500 ‚ slightly larger beam than incident beam‚ prevent from reaching transducer by a small negative bias
- X-ray emission‚ characteristic line spectra and continuum are produced
(1) column hosts the electron beam.(2) microscope is operated from the steering
panel(3) cryo-unit with a binocular (4) exchange chamber is used to introduce the
object into the high vacuum area. (5) The object can be observed on the large
screen while it is scanned. (6) The small screen serves to watch the object
chamber. (7) The computer for image archiving and
processing. (8) electronics
5. Scanning Probe Microscopes- resolve details of surface to the atomic level
‚ Nobel Prize in 1986 fro G. Binnig and H. Roher- provides details in x, y and z dimension
‚ 20 resolution in x, y as low as 1 ‚ resolution in z better than 1 ‚ electron microscope resolution is 50
direct observation of standing-wave patterns in the local density of states of the Cu(111) surface. These spatial oscillations are quantum-mechanical interference patterns caused by scattering of the two-dimensional electron gas off the Fe atoms and point defects.
A). Scanning Tunneling Microscopei. Introduction
- surface must conduct electricity- surface is scanned in raster pattern with a very fine metallic tip
- tip is maintained at constant distance from sample by maintaining a constant tunneling current ‚ up and down motion of tip reflects topology of surface‚ tunneling current created by voltage between tip and sample
STM tip scanning graphite surface (spheres are carbon atoms)
Scanned graphite surface
VConstant (d)
ii. Tunneling current- current that passes through a medium that contains no electrons‚ vacuum, nonpolar liquid, aqueous electrolyte solution‚ explained by quantum mechanics
- tunneling currents become significant when‚ two conductors are within a few nanometers of each other‚ one conductor is in the form of a sharp tip
- tunneling current (It) is given by:
It = Ve-Cd
where:V – voltage between conductorsC – constant dependent on composition of conductorsd – spacing between tip and surface
- tunneling current is held by moving tip up and down so d is constant ‚ tip is moved by potential change in x, y or z dimension that causes a hollow-tude piezoelectric device to bend in the x,y plane or extend/shrink along z-axis
Image of STM Tip
The inner and outer curved surfaces are coated with a thin metal layer to form two electrodes. The piezo tube bends under application of unequal voltages to the electrodes. Accuracy of movement is on the order of 1 nm
SEM used to move Fe atoms
iii. Tips- critical to performance of SEM- best images when the end of the tip is a single metal atom‚ tunneling current increases by 10x when gap distance decreases by 1 ‚ all current flows to single atom that is 1 closer to surface than all other atoms
- tips constructed by: ‚ cutting platinum/iridium wires‚ electrochemical etching of tungsten metal‚ exponential increase in tunneling current with decreasing gap makes it possible to prepare single atom tip Image of STM Tip
B). Atomic Force Microscope (AFM)i. Introduction
- resolution of individual atoms on both conducting and insulating surfaces ‚ STM requires conducting surface
- flexible force-sensing cantilever stylus is scanned over the surface- force acting between cantilever and surface causes minute deflections of the cantilever ‚ deflections detected by optical means‚ motion of cantilever controlled by piezoelectric tube (same as STM)
1. Laser 2. Mirror 3. Photodetector 4. Amplifier 5. Register 6. Sample 7. Probe 8. Cantilever
Bending or tapping of cantilever as it moves across service
Images of cantilever and tip
- laser beam is reflected off a spot on the cantilever to photodiode that detects the motion
‚ output from phtodiode then controls force on cantilever- output from photodiode then controls force on cantilever so that it remains constant
‚ similar to tunneling current control in STM‚ motion of cantilever controlled by piezoelectric tube (same as STM)
ii. Tips and Cantilever- critical to performance of AFM- originally crushed diamonds attached to metal foil
- currently, tips constructed by: ‚ etching single chips of silicon, silicon oxide or silicon nitride‚ remarkably small and delicate
- few tens of m in length, less then 10 m in width, ~ 1 m thickness- tips are few m in height and width
Can view cantilever as coil spring
iii. Tapping Mode Operation- disadvantages of contact mode scanning‚ potential damage of surface and distortion of image‚ especially problematic with “soft” samples
- biological samples- polymers- silicon wafers
- Tapping mode ‚ only allow tip to contact surface briefly then removed from surface ‚ cantilever oscillates at frequency of few 100 kHz ‚ image material that was impossible to image by contact mode
Atomic force microscopy images of reconstituted nucleosomal arrays. (A) A chromatin fiber with a beads-on-a-string morphology reconstituted at 1 : 1 histone octamers to DNA ratio. (B) When 1.5 : 1 histone octamers to DNA ratio is used for reconstitution a condensation of the core histone octamers is observed
Recommended